ASTM
A333G1
Standard specification for seamless and welded steel pipe (Low Temperature)
Outside
Diameter: 1/8 – 26 (Nominal)
OD Tolerance: +/- 1%
Wall thickness: Scheduled
Wall Tolerance: +/- 12.5%
Impact
Requirements: -50 degrees F, -45 degrees C
Minimum Yield: 30,000 PSI
Minimum Tensile: 55,000 PSI
| Chemical Requirements: | C (max) | Mn | P (max) | S (max) | Si (min) | Cr (max) | Cu (max) | Mo (max) | Ni (max) | V (max) |
| % | .30 | .40-1.06 | .025 | .025 | - | - | - | - | - | - |
Hydrostatic Test
ASTM A333G3
Impact Requirements: -150 degrees F, -100 degrees C
Minimum Yield: 35,000 PSI
Minimum Tensile: 65,000 PSI
| Chemical Requirements: | C (max) | Mn | P (max) | S (max) | Ni | Si (min) | Cr (max) | Cu (max) | Mo (max) | Al | V (max) |
| % | .19 | .31- .64 | .025 | .025 | 3.18 - 3.82 | .18 - .37 | - | - | - | - | - |
ASTM
A333G4
Impact
Requirements: -150 degrees F, -100 degrees C
Minimum Yield: 35,000 PSI
Minimum Tensile: 60,000 PSI
| Chemical Requirements: | C (max) | Mn | P (max) | S (max) | Si (min) | Cr (max) | Cu (max) | Al | Ni (max) | V (max) |
| % | .12 | .50-1.05 | .025 | .025 | .08 - .37 | .44 - 1.01 | .4 - .75 | .04 - .3 | .47 - .98 | - |
ASTM
A333G6
Impact
Requirements: -50 degrees F, -45 degrees C
Minimum Yield: 35,000 PSI
Minimum Tensile: 60,000 PSI
| Chemical Requirements: | C (max) | Mn | P (max) | S (max) | Si (min) | Cr (max) | Cu (max) | Al | Ni (max) | V (max) |
| % | .3 | .29-1.06 | .025 | .025 | .1 | - | - | - | - | - |
ASTM
A333G7
Impact
Requirements: -50 degrees F, -45 degrees C
Minimum Yield: 35,000 PSI
Minimum Tensile: 65,000 PSI
| Chemical Requirements: | C (max) | Mn (max) | P (max) | S (max) | Si (min) | Cr (max) | Cu (max) | Mo (max) | Ni | V (max) |
| % | .19 | .9 | .025 | .025 | .13 - .32 | - | - | - | 2.03 - 2.57 | - |
ASTM
A333G8
Impact
Requirements: -320 degrees F, -195 degrees C
Minimum Yield: 75,000 PSI
Minimum Tensile: 100,000 PSI
| Chemical Requirements: | C (max) | Mn (max) | P (max) | S (max) | Si | Cr | Cu | Mo | Ni | V |
| % | .13 | .9 | .025 | .025 | .13 - .32 | - | - | - | 8.4 - 9.6 | - |
ASTM
A333G9
Impact
Requirements: -100 degrees F, -75 degrees C
Minimum Yield: 46,000 PSI
Minimum Tensile: 63,000 PSI
| Chemical Requirements: | C (max) | Mn | P (max) | S (max) | Si | Cr | Cu | Mo | Ni | V (max) |
| % | .20 | .40 - 1.06 | .025 | .025 | - | - | .75 - 1.25 | - | 1.60 - 2.24 | - |
ASTM
A333G10
Impact
Requirements: -75 degrees F, -60 degrees C
Minimum Yield: 65,000 PSI
Minimum Tensile: 80,000 PSI
| Chemical Requirements: | C (max) | Mn | P (max) | S (max) | Si | Cr (max) | Cu (max) | Mo (max) | Ni (max) | Nb | V (max) |
| % | .20 | 1.15 - 1.50 | .035 | .015 | .10 - .35 | .15 | .15 | .05 | .25 | .05 | .12 |
ASTM
A333G11
Minimum Yield: 35,000 PSI
Minimum Tensile: 65,000 PSI
| Chemical Requirements: | C (max) | Mn (max) | P (max) | S (max) | Si (max) | Cr (max) | Cu | Mo (max) | Ni (max) | Nb | Co(max) |
| % | .10 | .60 | .025 | .025 | .35 | .50 | - | .05 | 35.0 - 37.0 | .50 | .50 |